My new boat started to develop blisters under the gunnel paint where the cover snaps are attached.
After the 2nd season of use, I brought this to the attention of the dealer and Legend boats up in Ontario.
This was last October and the manufacturer still hasn't come up with a plan to remedy the problem.
I did the usual Google research and sent the links to the service manager at my dealer.

Guy at Legend said he didn't want to talk directly with me and problem should be handled through dealer.
They also wanted me to tow the boat back to the dealer ( 180 miles round trip ) so techs could check for stray current, which I did while down anyway for winter servicing. No stray current from my motor.
They also suggested that it could be a stray current problem at the docks I frequent or stray current at local, marinas.
I explained that most of the small boat launches I use have no electrical services and anyway, I'm only there long enough to get my trailer and retrieve the boat.
Anyway I just contacted the General Manager of the dealership (member of family who owns the business) who acted as my salesman two years ago when I showed up while the sales staff were away at a boat show.
He says he will look into problem.

From what I read, we have to remove the snaps that screw directly into the painted aluminum gunnel, sand, prime and paint affected areas.
Then we have to find a suitable gasket or washer to isolate the snap and the aluminum and even coat the shafts of the attaching screw with liquid electrical tape or silicone to isolate them as possible.

My question is, can those self tapping screws be backed out of the aluminum and then be re-installed?
I broke two bits trying with a hand screwdriver last fall, so I google up higher rated impact type bits like the Makita Gold
That should hold up in my corded drill/driver.
Anyone ever attempt this.
  #2   Report Post  
posted to rec.boats
external usenet poster
 
First recorded activity by BoatBanter: Mar 2014
Posts: 811
Default Galvanic corrosion

On 5/15/2014 8:00 AM, True North wrote:
My new boat started to develop blisters under the gunnel paint where the cover snaps are attached.
After the 2nd season of use, I brought this to the attention of the dealer and Legend boats up in Ontario.
This was last October and the manufacturer still hasn't come up with a plan to remedy the problem.
I did the usual Google research and sent the links to the service manager at my dealer.

Guy at Legend said he didn't want to talk directly with me and problem should be handled through dealer.
They also wanted me to tow the boat back to the dealer ( 180 miles round trip ) so techs could check for stray current, which I did while down anyway for winter servicing. No stray current from my motor.
They also suggested that it could be a stray current problem at the docks I frequent or stray current at local, marinas.
I explained that most of the small boat launches I use have no electrical services and anyway, I'm only there long enough to get my trailer and retrieve the boat.
Anyway I just contacted the General Manager of the dealership (member of family who owns the business) who acted as my salesman two years ago when I showed up while the sales staff were away at a boat show.
He says he will look into problem.

From what I read, we have to remove the snaps that screw directly into the painted aluminum gunnel, sand, prime and paint affected areas.
Then we have to find a suitable gasket or washer to isolate the snap and the aluminum and even coat the shafts of the attaching screw with liquid electrical tape or silicone to isolate them as possible.

My question is, can those self tapping screws be backed out of the aluminum and then be re-installed?
I broke two bits trying with a hand screwdriver last fall, so I google up higher rated impact type bits like the Makita Gold
That should hold up in my corded drill/driver.
Anyone ever attempt this.


Aluminum and stainless steel fasteners don't play well together,
usually. I have seen situations where a white substance builds up
between the aluminum and stainless fastener, making it difficult or
impossible to remove the fastener. There are different grades of
aluminum as well as stainless. The paint adds another dimention to the
problem. Your builder hit upon the wrong combination. He should have
known better. Is your boat certified for use in salt water? I would go
to a local aluminum salt water boat dealer and seek his help.
  #3   Report Post  
posted to rec.boats
external usenet poster
 
First recorded activity by BoatBanter: Jul 2006
Posts: 10,492
Default Galvanic corrosion

On Thu, 15 May 2014 05:00:06 -0700 (PDT), True North
wrote:

My new boat started to develop blisters under the gunnel paint where the cover snaps are attached.
After the 2nd season of use, I brought this to the attention of the dealer and Legend boats up in Ontario.
This was last October and the manufacturer still hasn't come up with a plan to remedy the problem.
I did the usual Google research and sent the links to the service manager at my dealer.

Guy at Legend said he didn't want to talk directly with me and problem should be handled through dealer.
They also wanted me to tow the boat back to the dealer ( 180 miles round trip ) so techs could check for stray current, which I did while down anyway for winter servicing. No stray current from my motor.
They also suggested that it could be a stray current problem at the docks I frequent or stray current at local, marinas.
I explained that most of the small boat launches I use have no electrical services and anyway, I'm only there long enough to get my trailer and retrieve the boat.
Anyway I just contacted the General Manager of the dealership (member of family who owns the business) who acted as my salesman two years ago when I showed up while the sales staff were away at a boat show.
He says he will look into problem.

From what I read, we have to remove the snaps that screw directly into the painted aluminum gunnel, sand, prime and paint affected areas.
Then we have to find a suitable gasket or washer to isolate the snap and the aluminum and even coat the shafts of the attaching screw with liquid electrical tape or silicone to isolate them as possible.

My question is, can those self tapping screws be backed out of the aluminum and then be re-installed?
I broke two bits trying with a hand screwdriver last fall, so I google up higher rated impact type bits like the Makita Gold
That should hold up in my corded drill/driver.
Anyone ever attempt this.


===

This is a big problem with aluminum sailboat masts and booms where
stainless steel screws and machine screws are used to attach fittings.
I once asked a professional rigger what he recommended and he said
that he always beds the hardware and threads with silicone sealant
before fastening. The silicone creates a thin insulating barrier
between the two metals and prevents corrosion. I've removd hardware
installed that way more than 5 years ago with no problems.

Removing old fasteners that have already corroded is difficult.
Frequently you have to break them off and punch them out. You can
build up the old hole with JB Weld or similar and then retap the
threads if the fasteners are not under a lot of stress.
  #4   Report Post  
posted to rec.boats
external usenet poster
 
First recorded activity by BoatBanter: Mar 2008
Posts: 216
Default Galvanic corrosion

On Thursday, May 15, 2014 11:45:06 AM UTC-4, Wayne. B wrote:
On Thu, 15 May 2014 05:00:06 -0700 (PDT), True North

wrote:



My new boat started to develop blisters under the gunnel paint where the cover snaps are attached.


After the 2nd season of use, I brought this to the attention of the dealer and Legend boats up in Ontario.


This was last October and the manufacturer still hasn't come up with a plan to remedy the problem.


I did the usual Google research and sent the links to the service manager at my dealer.




Guy at Legend said he didn't want to talk directly with me and problem should be handled through dealer.


They also wanted me to tow the boat back to the dealer ( 180 miles round trip ) so techs could check for stray current, which I did while down anyway for winter servicing. No stray current from my motor.


They also suggested that it could be a stray current problem at the docks I frequent or stray current at local, marinas.


I explained that most of the small boat launches I use have no electrical services and anyway, I'm only there long enough to get my trailer and retrieve the boat.


Anyway I just contacted the General Manager of the dealership (member of family who owns the business) who acted as my salesman two years ago when I showed up while the sales staff were away at a boat show.


He says he will look into problem.




From what I read, we have to remove the snaps that screw directly into the painted aluminum gunnel, sand, prime and paint affected areas.


Then we have to find a suitable gasket or washer to isolate the snap and the aluminum and even coat the shafts of the attaching screw with liquid electrical tape or silicone to isolate them as possible.




My question is, can those self tapping screws be backed out of the aluminum and then be re-installed?


I broke two bits trying with a hand screwdriver last fall, so I google up higher rated impact type bits like the Makita Gold


That should hold up in my corded drill/driver.


Anyone ever attempt this.




===



This is a big problem with aluminum sailboat masts and booms where

stainless steel screws and machine screws are used to attach fittings.

I once asked a professional rigger what he recommended and he said

that he always beds the hardware and threads with silicone sealant

before fastening. The silicone creates a thin insulating barrier

between the two metals and prevents corrosion. I've removd hardware

installed that way more than 5 years ago with no problems.




I'm doubtful that anything actually prevents the two metals from connecting.. I suggest you try a simple ohm meter test to prove that to yourself. Rather the silicon is reducing the moisture reaching the joint. If you can keep the water out you will greatly reduce the corrosion. Personally I use teflon thread sealer on everything threaded. It too will help keep the water out as well as lubricate the threads. Stainless is the best hardware since aluminum fasteners would generally be too weak.
  #5   Report Post  
posted to rec.boats
external usenet poster
 
First recorded activity by BoatBanter: Jul 2006
Posts: 10,492
Default Galvanic corrosion

On Thu, 15 May 2014 11:59:49 -0700 (PDT), wrote:

On Thursday, May 15, 2014 11:45:06 AM UTC-4, Wayne. B wrote:
On Thu, 15 May 2014 05:00:06 -0700 (PDT), True North

wrote:



My new boat started to develop blisters under the gunnel paint where the cover snaps are attached.


After the 2nd season of use, I brought this to the attention of the dealer and Legend boats up in Ontario.


This was last October and the manufacturer still hasn't come up with a plan to remedy the problem.


I did the usual Google research and sent the links to the service manager at my dealer.




Guy at Legend said he didn't want to talk directly with me and problem should be handled through dealer.


They also wanted me to tow the boat back to the dealer ( 180 miles round trip ) so techs could check for stray current, which I did while down anyway for winter servicing. No stray current from my motor.


They also suggested that it could be a stray current problem at the docks I frequent or stray current at local, marinas.


I explained that most of the small boat launches I use have no electrical services and anyway, I'm only there long enough to get my trailer and retrieve the boat.


Anyway I just contacted the General Manager of the dealership (member of family who owns the business) who acted as my salesman two years ago when I showed up while the sales staff were away at a boat show.


He says he will look into problem.




From what I read, we have to remove the snaps that screw directly into the painted aluminum gunnel, sand, prime and paint affected areas.


Then we have to find a suitable gasket or washer to isolate the snap and the aluminum and even coat the shafts of the attaching screw with liquid electrical tape or silicone to isolate them as possible.




My question is, can those self tapping screws be backed out of the aluminum and then be re-installed?


I broke two bits trying with a hand screwdriver last fall, so I google up higher rated impact type bits like the Makita Gold


That should hold up in my corded drill/driver.


Anyone ever attempt this.




===



This is a big problem with aluminum sailboat masts and booms where

stainless steel screws and machine screws are used to attach fittings.

I once asked a professional rigger what he recommended and he said

that he always beds the hardware and threads with silicone sealant

before fastening. The silicone creates a thin insulating barrier

between the two metals and prevents corrosion. I've removd hardware

installed that way more than 5 years ago with no problems.




I'm doubtful that anything actually prevents the two metals from connecting.
I suggest you try a simple ohm meter test to prove that to yourself. Rather
the silicon is reducing the moisture reaching the joint. If you can keep the water
out you will greatly reduce the corrosion. Personally I use teflon thread sealer on
everything threaded. It too will help keep the water out as well as lubricate the
threads. Stainless is the best hardware since aluminum fasteners would generally be too weak.


===

Although the exact protection mechanism may be debatable, it has been
well proven that anything that prevents direct contact between
dissimilar metals helps to prevent corrosion.


  #6   Report Post  
posted to rec.boats
Banned
 
First recorded activity by BoatBanter: Jun 2013
Posts: 1,692
Default Galvanic corrosion

On Thursday, May 15, 2014 8:00:06 AM UTC-4, True North wrote:
My new boat started to develop blisters under the gunnel paint where the cover snaps are attached.

After the 2nd season of use, I brought this to the attention of the dealer and Legend boats up in Ontario.

This was last October and the manufacturer still hasn't come up with a plan to remedy the problem.

I did the usual Google research and sent the links to the service manager at my dealer.



Guy at Legend said he didn't want to talk directly with me and problem should be handled through dealer.

They also wanted me to tow the boat back to the dealer ( 180 miles round trip ) so techs could check for stray current, which I did while down anyway for winter servicing. No stray current from my motor.

They also suggested that it could be a stray current problem at the docks I frequent or stray current at local, marinas.

I explained that most of the small boat launches I use have no electrical services and anyway, I'm only there long enough to get my trailer and retrieve the boat.

Anyway I just contacted the General Manager of the dealership (member of family who owns the business) who acted as my salesman two years ago when I showed up while the sales staff were away at a boat show.

He says he will look into problem.



From what I read, we have to remove the snaps that screw directly into the painted aluminum gunnel, sand, prime and paint affected areas.

Then we have to find a suitable gasket or washer to isolate the snap and the aluminum and even coat the shafts of the attaching screw with liquid electrical tape or silicone to isolate them as possible.



My question is, can those self tapping screws be backed out of the aluminum and then be re-installed?

I broke two bits trying with a hand screwdriver last fall, so I google up higher rated impact type bits like the Makita Gold

That should hold up in my corded drill/driver.

Anyone ever attempt this.


Too bad your $16,000 dollar Bass Boat is corroding. Looks real good on you.
After all, you are totally ****ing stupid, and cant even back up a trailered Boat.
  #8   Report Post  
posted to rec.boats
Banned
 
First recorded activity by BoatBanter: Jun 2013
Posts: 1,692
Default Galvanic corrosion

On Friday, May 16, 2014 10:30:05 AM UTC-4, wrote:

The first thing Don has to do is be sure these are really stainless

and not chrome over brass.


He's TOO ****ING STUPID TO TELL THE DIFFERENCE.
  #9   Report Post  
posted to rec.boats
external usenet poster
 
First recorded activity by BoatBanter: Jan 2011
Posts: 5,756
Default Galvanic corrosion

Yesterday I was on the Legend website where they have a chat function.
I asked the rep about the snaps and she confirmed that they were indeed stainless steel.
She then asked if I had any other concerns.
I felt chatty so I informed her about the corrosion problem... not really expecting to much back.
She went right to the warranty manager and quoted him as saying salt water corrosion was an unpredictable process and not really a warranty problem. He also stated they didn't recommend their boats be used in salt water.
First I heard of this and no where have I seen this in writing nor did the dealer mention it.
They did say to forward pictures of the blisters and they would consult with the dealer on what to do.
Looks like I may be looking for a good Jewish lawyer.
  #10   Report Post  
posted to rec.boats
external usenet poster
 
First recorded activity by BoatBanter: Mar 2014
Posts: 811
Default Galvanic corrosion

On 5/17/2014 6:33 AM, True North wrote:
Yesterday I was on the Legend website where they have a chat function.
I asked the rep about the snaps and she confirmed that they were indeed stainless steel.
She then asked if I had any other concerns.
I felt chatty so I informed her about the corrosion problem... not really expecting to much back.
She went right to the warranty manager and quoted him as saying salt water corrosion was an unpredictable process and not really a warranty problem. He also stated they didn't recommend their boats be used in salt water.
First I heard of this and no where have I seen this in writing nor did the dealer mention it.
They did say to forward pictures of the blisters and they would consult with the dealer on what to do.
Looks like I may be looking for a good Jewish lawyer.

A good Jewish lawyer wouldn't take your case. If you want to prevent
further disintegration of your boat, don't use it in salt water. Do you
know what the third least noble metal next to lead and magnesium is?
Hint. It's one of the materials that Mercury Marine recommends as a
sacrificial anode.
Reply
Thread Tools Search this Thread
Search this Thread:

Advanced Search
Display Modes

Posting Rules

Smilies are On
[IMG] code is Off
HTML code is Off
Trackbacks are On
Pingbacks are On
Refbacks are On


Similar Threads
Thread Thread Starter Forum Replies Last Post
Severe galvanic corrosion video Chuck General 18 September 15th 08 02:21 AM
Corrosion - Good Products to Remove Aluminum Corrosion ? B1ackwater General 8 March 31st 06 12:48 AM
Galvanic corrosion and Radio Brian Reay Electronics 5 January 22nd 05 09:21 PM
Seamanship Question #17 Galvanic Corrosion N1EE ASA 9 December 3rd 04 12:28 AM
galvanic corrosion Jean Electronics 2 October 8th 03 02:58 PM


All times are GMT +1. The time now is 12:41 AM.

Powered by vBulletin® Copyright ©2000 - 2025, Jelsoft Enterprises Ltd.
Copyright ©2004-2025 BoatBanter.com.
The comments are property of their posters.
 

About Us

"It's about Boats"

 

Copyright © 2017